UP 5690-W or-K POLYOL |
UP 5690 ISOCYANATE |
UP 5690 C |
MIXED |
| Composition |
|
Polyol |
Isocyanate |
Polyol |
|
| Mix ratio by weight |
|
100 |
100 |
0 - 50 |
|
| Aspect |
|
liquid |
liquid |
liquid |
liquid |
| Colour |
|
W= WhiteK= Black |
Colourless |
Milk white |
AW/B/C=White AK/B/C=Black |
| Viscosity at 23°C (mPa.s) |
BROOKFIELD LVT |
1000 - 1500 |
140 - 180 |
4500 - 5000 |
500 - 700 |
| Viscosity at 40°C (mPa.s) |
BROOKFIELD LVT |
400 - 600 |
- |
2300 - 2500 |
300 - 500 |
| Specific gravity at 25°CSpecific gravity of curedproduct at 23°C |
ISO 1675 :1975 ISO 2781 :1988 |
1.06- |
1.15- |
1.06- |
-1.13 |
| Pot life at 25°C on 100 g (min) |
|
|
|
|
10 - 15 |
| Pot life at 40°C on 100 g (min) |
|
|
|
|
5 - 7 |
PROCESSING CONDITIONS (Vacuum casting machine)
• Preheat isocyanate to 23 - 30°C in case of being stored below 20°C .
• Preheat polyol and part C to 40°C before using. It is necessary to stir the polyol until both color and aspect become homogeneous.
• Weigh the components according to the mixing ratio, put isocyanate into the upper cup, add part C in polyol to premix.
• Pour isocyanate into polyol (containing Part C) and mix for 1 - 2 minutes after degassing for 10 minutes seperately.
• Cast under vacuum in silicone mould preheated to 70°C.
• Demould after 60 - 90 minutes at 70°C (The more Part C is used, the longer demoulding time is needed)..
| A/B/C |
100/100/0 |
100/100/20 |
100/100/30 |
100/100/50 |
| Hardness |
ISO 868 : 2003 |
Shore D |
83 |
80 |
78 |
75 |
| Tensile strength |
ISO 527 : 1993 |
MPa |
35 |
30 |
28 |
25 |
| Flexural strength |
ISO 178 : 2001 |
MPa |
50 |
35 |
30 |
20 |
| Flexural modulus |
ISO 178 : 2001 |
MPa |
1300 |
1000 |
900 |
600 |
| Elongation at break |
ISO 527 : 1993 |
% |
50 |
60 |
65 |
90 |
| Impact strength(CHARPY)Unnotched specimens |
ISO 179/2D : 1994 |
KJ/m2 |
100 |
90 |
85 |
75 |
| A/B/C |
100/100/0 |
100/100/20 |
100/100/30 |
100/100/50 |
| Glass transition temperature (Tg) |
(1) |
°C |
85 |
78 |
75 |
65 |
| Linear shrinkage |
% |
0.35 |
0.35 |
0.35 |
0.35 |
| Demoulding time (2 - 3mm) at 70°C |
min |
60 - 90 |
Average values obtained on standard specimens / Hardening 16hr at 80°C after demoulding.
Handling Precautions
Normal health and safety precautions should be observed when handling these products :
Ensure good ventilation
Wear gloves, safety glasses and protective clothes.
For further information, please consult the product safety data sheet.
Storage Conditions
Shelf life is 6 months in a dry place and in original unopened containers at a temperature between 15 and 25° C. Any open can must be tightly closed under dry nitrogen blanket.
High Mechanical Vacuum CastPP likeVacuum Casting PP like
High Mechanical Strength Light Weight Vacuum Casting PP like Related Video: